1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
K-001
Objective is to produce a functional knife stepping through the process using blockchain only as a means of recording with video clips and pictures.
I have all the gear and no idea so will just make things up as it progresses.
Replies
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
1.
The process begins with obtaining stock. Damascus steel is being used
The first task is to make the stock flat enough to obtain the blade
Each side is cut repeatedly bit by bit so as to account for material stresses
The stock is hand made and not flat
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
2.
In CNC milling 'part probing' is a useful function that enables both location and measurement of the part to be worked upon.
In this case a Renishaw setter capable of measuring down to the micron is used.
The process is repeated many times until flat.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
3.
A quiet week but weekend is coming.
I test how proper metal bends with a 100lb load.
Cut some scrap stainless to make handles to test how they feel. The handles at this time weigh 1lb or 450 grams.
I order solid copper stock to make final handles.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
4.
Settle on a final idea and begin to make stuff now.
It is going to be simple and very heavy. At a minimum a nice paper weight.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
5.
The best part of a weekend and only half a handle
I have no spare stock so it has to be correct first time in this trial
Most of the time goes in to tooling and part holding
It looks small but all the bits are required to be assembled before judgement
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
6.
Preparing blade blanks.
Material availability restricted efficient part nesting.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
7.
First blank processed but only insofar as the profile and handle fitment.
Tool pressure was enough to overcome magnetic holding resulting in the blade moving and an out of spec part. Solution is to reduce pressure by doing multiple laps around the part
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
8.
Still no good, another out of spec example (should be 14.9mm).
This magnetic holding simply isn't up to the task of managing the smallest of loads with profile cutting
Plan now is to cut to exact size from the stock plate as in (6.) instead of trimming
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
9.
Air quality.
The problem with doing this kind of work in the small home workshop is that high speed spindles + coolant produce atomised oil vapours that coat everything else in the workshop.
A means of preventing this is required.
Testing.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
10.
A couple of weeks and things have gone full circle back to the beginning. Trying to hold vibrating things with magnets isn't any good. There are a couple of feel type things to change in the design then run it again and see what happens.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
11.
A few minor changes to the blade, radius, move 1st bolt hole for strength
Use magnet and clamps
Keep blades inside stock for larger clamping surfaces
Optimise machining strategy, looking better now
Through holes A and B help find part zero when flipped
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
12.
Process stability
With automated manufacture process stability is important. If a cutter breaks early on in an unattended process it is possible other cutters will also break as they plunge in to material that should have been removed
All good here now
1NnsVVVj5X2hid579uqVcRCf7s2TcqEVG ·
Are you planning to sell these once you work out all the manufacturing details? How about making other shapes. Are you going to make a set? I use a cleaver about 90% of the time, rarely grab the butcher knife.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
1
These are not economically viable, by a quite a margin
I do it just for fun and to learn something I have not done before
There will be a small number of them and I will give them away
This isn't really costing as it is reallocated small blocker funds😁
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
2
Been meaning to do something like this for a long time but motivation issues where I can't be bothered to do more work outside of work.
I still have a home brew CNC lathe to complete along with getting the workshop lean where hoarding can be problematic.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
Loafing cat on the lookout now as a reminder.
1NnsVVVj5X2hid579uqVcRCf7s2TcqEVG ·
That CNC could cut out a nice styalized guitar bridge. It’s hard to find the perfect aesthetics for a custom build. Making custom designs would open up so many options. Custom knobs and scratch plates too. Lots of possibilities.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
I know.
I could see you had an eye for detail a long time back.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
13.
Chump
Upside down and 180 out on the rotation. Not done this in a long while. In the bin.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
Might as well get the dog to do it but as usual she only wants treats.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14a
Heat treating
Had to wait a couple of weeks for some stainless foil to arrive
Talc is used to prevent the blade sticking to the foil
I saw someone using wood as means of oxygen scavenging which does not work
2 samples were tested with slight variations
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14b
First blade
Heat to 1050C Temper at 185C for two 2 hour sessions.
Wood gas caused foil bag to expand and some oxidisation was present.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14c
Second blade
Heat to 1050C Temper at 190C for two 2 hour sessions.
The foil bag was made much tighter with less void space for oxygen, Oxidisation was minimal.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14d
Destructive testing (scrap blades)
The first step was to test the metal as delivered with no heat treat so as to establish a general baseline.
File it bend it.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14e
First blade destructive test.
It passed the file test but seemed a little too brittle. The metal had the nice tight ring to it characteristic of bearings and the like which are high hardness metals. The flying bit did put a hole in the wall.
1HqqhgFgy8ppM5p7kjd3A5KiJBaYYkfzmw ·
14f
The second blade seemed just about right, perhaps raising the temper temperature up to 200C may give a little more flex. The blade did bend and stayed bent indicating a step down from full hardness.
The more technical bit of blade making is simple.